No.
|
Kuat Tekan (kg/cm2)
|
|||||||||
Normal
|
200oC
|
250oC
|
300oC
|
350oC
|
400oC
|
450oC
|
500oC
|
550oC
|
600oC
|
|
1.
|
239.63
|
221.34
|
134.80
|
151.99
|
142.54
|
134.23
|
130.45
|
100.47
|
93.67
|
99.54
|
2.
|
265.43
|
220.75
|
209.96
|
151.99
|
143.78
|
146.44
|
133.41
|
105.61
|
102.73
|
61.81
|
3.
|
229.58
|
183.22
|
165.13
|
151.99
|
140.34
|
151.81
|
130.36
|
76.96
|
78.89
|
100.88
|
4.
|
235.14
|
211.22
|
131.15
|
151.99
|
147.90
|
144.73
|
120.40
|
114.79
|
99.67
|
62.11
|
5.
|
250.85
|
233.71
|
155.56
|
151.99
|
160.61
|
141.29
|
137.78
|
108.45
|
107.82
|
105.82
|
6.
|
237.65
|
198.90
|
133.34
|
151.99
|
143.01
|
136.88
|
126.60
|
108.45
|
92.42
|
92.59
|
7.
|
244.01
|
198.68
|
206.40
|
151.99
|
147.90
|
149.12
|
131.31
|
79.47
|
99.67
|
68.77
|
8.
|
266.19
|
189.85
|
135.45
|
151.99
|
154.53
|
140.35
|
122.56
|
103.75
|
97.45
|
102.04
|
9.
|
247.73
|
200.42
|
133.41
|
151.99
|
139.42
|
144.25
|
138.24
|
110.01
|
87.43
|
99.34
|
10.
|
239.63
|
242.53
|
189.15
|
151.99
|
153.50
|
145.05
|
132.45
|
104.84
|
98.03
|
68.57
|
Salah satu
tantangan yang dihadapi para ahli struktur (teknik sipil) adalah bagaimana
menaksir:
a) temperatur
tertinggi yang pernah dialami elemen bangunan pada saat kebakaran terjadi
b) kekuatan
sisa bangunan pasca kebakaran, dan
c) teknik perkuatan bangunan sesuai keperluan sehingga
fungsi bangunan dapat dikembalikanseperti sebelum kebakaran.
Untuk
menjawab secara ilmiah tantangan tersebut sekaligus membantu masyarakat dalam
menangani masalah ini secara tepat, telah dikembangkan berbagai metode
penaksiran. Metode ini digunakan untuk dapat memperkirakan secara akurat
temperatur tertinggi yang pernah dialami bangunan, kekuatan sisa struktur
bangunan pasca kebakaran, dan teknik perkuatan bangunannya. Berbagai masalah
teknik yang menyangkut penaksiran kekuatan sisa dan teknik perkuatan elemen
struktur tersebut hasilnya dimanfaatkan oleh pihak lain yang terkait, seperti
pemilik bangunan, pihak kepolisian, pengacara hukum, dan perusahaan asuransi.
Sampai saat ini penelitian tentang
pengaruh temperatur pada beton masih merupakan topik yang hangat diteliti.
Pengaruh temperatur diukur, baik sifat fisik maupun sifat mekanik, dan
dianalisis dengan menggunakan analisis statistik deskriptif. Keinginan para
peneliti untuk mengetahui secara akurat bentuk, gambaran, dan seberapa besar
pengaruh temperatur terhadap beton merupakan hal yang masih ingin diketahui sampai
saat ini. Para peneliti mulai meneliti dengan membuat benda uji beton yang
kemudian dibakar langsung atau dibakar dalam oven atau tungku. Setelah itu,
dilakukan pengujan pada benda uji berupa kuat tekan, kuat lentur, dan modulus
elastisitas. Semua penelitian yang dilakukan merupakan usaha untuk menaksir
kekuatan sisa suatu bangunan yang telah terbakar. Namun sejauh ini penelitian
penaksiran tersebut masih belum menemukan landasan awal yang kuat.
Metode analisis yang digunakan
adalah analisis statistik deskriptif, menggambarkan bagaimana kuat tekan beton
setelah pemanasan. Sedangkan untuk mengetahui model hubungan temperatur dan
kuat tekan beton digunakan analisis regresi.
Berdasarkan data makalah “Pengaruh Temperatur terhadap Kuat Tekan Beton” adalah sebagai berikut :
No.
|
Kuat Tekan
(kg/cm2)
|
|||||||||
Normal
|
200oC
|
250oC
|
300oC
|
350oC
|
400oC
|
450oC
|
500oC
|
550oC
|
600oC
|
|
1.
|
239.63
|
221.34
|
134.80
|
151.99
|
142.54
|
134.23
|
130.45
|
100.47
|
93.67
|
99.54
|
2.
|
265.43
|
220.75
|
209.96
|
151.99
|
143.78
|
146.44
|
133.41
|
105.61
|
102.73
|
61.81
|
3.
|
229.58
|
183.22
|
165.13
|
151.99
|
140.34
|
151.81
|
130.36
|
76.96
|
78.89
|
100.88
|
4.
|
235.14
|
211.22
|
131.15
|
151.99
|
147.90
|
144.73
|
120.40
|
114.79
|
99.67
|
62.11
|
5.
|
250.85
|
233.71
|
155.56
|
151.99
|
160.61
|
141.29
|
137.78
|
108.45
|
107.82
|
105.82
|
6.
|
237.65
|
198.90
|
133.34
|
151.99
|
143.01
|
136.88
|
126.60
|
108.45
|
92.42
|
92.59
|
7.
|
244.01
|
198.68
|
206.40
|
151.99
|
147.90
|
149.12
|
131.31
|
79.47
|
99.67
|
68.77
|
8.
|
266.19
|
189.85
|
135.45
|
151.99
|
154.53
|
140.35
|
122.56
|
103.75
|
97.45
|
102.04
|
9.
|
247.73
|
200.42
|
133.41
|
151.99
|
139.42
|
144.25
|
138.24
|
110.01
|
87.43
|
99.34
|
10.
|
239.63
|
242.53
|
189.15
|
151.99
|
153.50
|
145.05
|
132.45
|
104.84
|
98.03
|
68.57
|
Dari data diatas
ditentukan rata-rata percobaan kuat tekan beton pada tiap temperatur:
No
|
Temperatur
|
Kuat Tekan Beton
|
1
|
25
|
245,584
|
2
|
200
|
210,062
|
3
|
250
|
159,435
|
4
|
300
|
151,99
|
5
|
350
|
147,353
|
6
|
400
|
143,415
|
7
|
450
|
130,356
|
8
|
500
|
101,28
|
9
|
550
|
95,778
|
10
|
600
|
86,147
|
∑
|
3625
|
1471,4
|
Ø Regresi Non Linier → Logaritmik
No
|
x
|
y
|
ln x
|
ln^2 x
|
ln x . Y
|
1
|
25
|
245,584
|
3,218876
|
10,36116
|
790,5044
|
2
|
200
|
210,062
|
5,298317
|
28,07217
|
1112,975
|
3
|
250
|
159,435
|
5,521461
|
30,48653
|
880,3141
|
4
|
300
|
151,99
|
5,703782
|
32,53313
|
866,9179
|
5
|
350
|
147,353
|
5,857933
|
34,31538
|
863,184
|
6
|
400
|
143,415
|
5,991465
|
35,89765
|
859,2659
|
7
|
450
|
130,356
|
6,109248
|
37,32291
|
796,3771
|
8
|
500
|
101,28
|
6,214608
|
38,62135
|
629,4155
|
9
|
550
|
95,778
|
6,309918
|
39,81507
|
604,3514
|
10
|
600
|
86,147
|
6,39693
|
40,92071
|
551,0763
|
∑
|
3625
|
1471,4
|
56,62254
|
328,3461
|
7954,382
|
titik koordinat y:
|
|
x=25 → y=
|
266,2493
|
x=200 → y=
|
164,8811
|
x=250 → y=
|
154,0033
|
x=300 → y=
|
145,1156
|
x=350 → y=
|
137,6011
|
x=400 → y=
|
131,0917
|
x=450 → y=
|
125,35
|
x=500 → y=
|
120,2139
|
x=550 → y=
|
115,5678
|
x=600 → y=
|
111,3262
|
Ø Regresi Non Linier → Eksponensial
No
|
x
|
y
|
ln x
|
ln y
|
xi.ln y
|
xi^2
|
1
|
25
|
245,584
|
3,218876
|
5,503639
|
137,591
|
625
|
2
|
200
|
210,062
|
5,298317
|
5,347403
|
1069,481
|
40000
|
3
|
250
|
159,435
|
5,521461
|
5,071636
|
1267,909
|
62500
|
4
|
300
|
151,99
|
5,703782
|
5,023815
|
1507,144
|
90000
|
5
|
350
|
147,353
|
5,857933
|
4,992831
|
1747,491
|
122500
|
6
|
400
|
143,415
|
5,991465
|
4,965743
|
1986,297
|
160000
|
7
|
450
|
130,356
|
6,109248
|
4,870269
|
2191,621
|
202500
|
8
|
500
|
101,28
|
6,214608
|
4,617889
|
2308,944
|
250000
|
9
|
550
|
95,778
|
6,309918
|
4,562033
|
2509,118
|
302500
|
10
|
600
|
86,147
|
6,39693
|
4,456055
|
2673,633
|
360000
|
∑
|
3625
|
1471,4
|
56,62254
|
49,41131
|
17399,23
|
1590625
|
sumber :
Suryaningsih T., N.
A., & Ahmad, I. A. (2009). Jurnal Teoretis dan Terapan Bidang Rekayasa
Sipil. Analisis Pengaruh Temperatur terhadap Kuat Tekan Beton.
Mhn dicantumkan Nama dan NRP, untuk dilakukan penilaian. Mhn dibuat grafik dari data tersebut dan dibuat analisa dari grafik tersebut?
BalasHapussudah saya cantumkan bapak, sudah saya tambahkan grafik dan analisa regresi non linier bapak, terimakasih
HapusApa yang dapat anda simpulkan dari kedua grafik tersebut ya dik?
Hapus